Structural Steel- Mechanical properties according to EN 10025-2:2004

Standard referred to: EN 10025-2:2004 Former references
Steel
grade

Minimum yield strength ReH

Tensile strength Rm

Minimum elongation
Lo = 5,65√So

F

NF A 35-501

D

DIN 1710

GB

BS 4360

B

NBN A21-101

Thickness

 

 

 

 

(N/mm2)

≤ 16

(N/mm2)

> 16
≤ 40

(N/mm2)

≥ 3
 ≤ 100

(mm) %

≥ 3
 ≤ 40

       
S 235 JR 235 225 340-470 26   RSt 37-2 40 B  
S 235 J0 235 225 340-470 26 E 24-3 St 37-3 U 40 C AE 235-C
S 275 JR 275 265 410-560 22 E 28-2 St 44-2 43 B AE 255-B
S 275 J0 275 265 410-560 22 E 28-3 St 44-3 U 43 C AE 255-C
S 355 JR 355 345 490-630 22 E 36-2   50 B AE 355-B
S 355 J0 355 345 490-630 22 E 36-3 St 52-3 U 50 C AE 355-C
S 355 J2 355 345 490-630 22   St 52-3 N 50 D AE 355-D

*Other steel grades can be delivered on request.

Mechanical properties according to EN EN 10025-4:2004

Standard referred to: EN 10025-4:2004 Comparable international standards
Steel
grade

Minimum yield strength ReH 

Epaisseur (mm) (N/mm2)

Tensile strength Rm (N/mm2)

Minimum elongation %

(Lo = 5,65√So)

USA

(ASTM)

Japan

(JIS G 3101)

≤ 16 > 16
≤ 40
S 355 M 355 345 450-610 22 A 913 Gr. 50  
S 355 ML 355 345 450-610 22    
S 460 M 460 440 530-720 17 A 913 Gr. 65 SM 570
S 460 ML 460 440 530-720 17    

HISTAR® steels- Outstanding weldability (carbon equivalent lower than 0.41 %).

HISTAR® Comparable international standards
Steel
grade
Minimum yield strength ReH (N/mm2) Tensile strength Rm (N/mm2) Minimum elongation
Lo = 5,65√So (%)
USA ASTM
A 572
A 913
USA ASTM
A 992
Japan JIS
G 3106
HISTAR 355 355 470-610 22 Gr. 50 Gr. 50 SM490B/C/YB
HISTAR 460 460 550-720 17 Gr. 65   SM570

For all HISTAR® grades: Charpy V notch impact test, longitudinal: ≥40 J at -20°C.